Ultrasonic and Eddy Current Testing of Steel Bar: Methods, Standards and Defects Found
Send an enquiryUltrasonic testing and eddy current testing are two non-destructive methods by which steel bar is examined over its length for defects that the eye and a dimensional check cannot find. Ultrasonic testing sends a beam of high-frequency sound into the bar and records the echoes returned by discontinuities inside it, so it examines the volume of the bar from below the surface to the centre. Eddy current testing induces an alternating electric current in the bar from a coil and records the disturbance that a discontinuity causes in that current, so it examines the surface and the layer just beneath it. A specification for bar that will be machined into a shaft, a valve stem or a highly stressed part may call for one or both, names the standard that governs the method, and states an acceptance level agreed between purchaser and supplier.
Internal and surface defects in bar
Internal defects in bar originate in solidification. A cast billet, bloom or ingot can carry a shrinkage cavity or porosity along its centreline, segregation of alloying and impurity elements toward the centre, and clusters of non-metallic inclusions. Rolling closes and elongates much of this material but does not always weld it shut, and a defect that survives rolling lies along the bar axis. Hydrogen dissolved in the steel can also produce internal hairline cracks, called flakes, in hydrogen-sensitive alloy steels as the bar cools. The article on ingots, blooms and billets describes these casting defects.
Surface defects originate mainly in hot rolling. A seam is a longitudinal crevice that is tight or closed at the surface but not welded shut, and rolling stretches it along the bar. A lap is a fold of metal: an overfill or fin formed in one pass and rolled back into the surface in a later one. Slivers, rolled-in scale and quench cracks are further surface defects. Peeling, turning and grinding remove a surface layer and with it any defect shallower than the stock removed; a deeper defect remains.
Ultrasonic testing: pulse-echo, frequency and coupling
Ultrasonic testing of bar uses the pulse-echo technique. A piezoelectric transducer emits a short pulse of longitudinal waves into the bar at right angles to the surface and then listens for echoes. Longitudinal waves travel at close to 5,900 metres per second in carbon and low-alloy steel and slightly more slowly in austenitic stainless steel, so the time between the transmitted pulse and an echo gives the depth of the reflector. A sound bar returns a strong echo from the far surface, the back wall. A discontinuity in the beam returns an earlier echo and may weaken the back-wall echo by intercepting part of the beam. The amplitude of the discontinuity echo, compared with the echo from a reference reflector at the same depth, gives its equivalent size.
The frequency sets the balance between resolution and penetration. A higher frequency gives a shorter wavelength and resolves smaller reflectors, but the sound is scattered more strongly by grain boundaries and penetrates less far. EN 10308 calls for probes with a nominal frequency between 1 and 6 MHz. Almost no sound crosses an air gap, so a couplant fills the space between probe and bar. In manual contact testing the couplant is a film of water, oil or gel. In automatic testing, water usually couples a set of probes to the moving bar without contact, which keeps the coupling stable at production speed.
Straight-beam testing sees the layer just below the entry surface poorly, because the transmitted pulse and the ringing of the probe mask early echoes. Double transducer probes, with separate transmitting and receiving elements, reduce this effect; EN 10308 permits them on bars up to 150 mm and calls for single transducer probes above 60 mm. The scanning surface must be free from paint, loose scale and other matter that would disturb coupling or cause false indications.
Standards for ultrasonic testing of bar
EN 10308, Non-destructive testing: Ultrasonic testing of steel bars, is the European standard for the method. It covers manual pulse-echo testing of round, square, rectangular and other bar sections up to 400 mm in diameter or equivalent thickness, with mechanised or automatic testing permitted by agreement. It requires a written procedure and lists the points to be agreed at the time of enquiry or order, among them the stage of manufacture, grid or complete scanning, the quality class and the zones to which it applies, and the method of setting sensitivity: a distance-amplitude curve from flat-bottomed holes, or the distance-gain-size method. Unless otherwise agreed, the test follows the final quality heat treatment. The standard recommends certification of personnel under EN 473, which ISO 9712 has since replaced.
ASTM E2375, Standard Practice for Ultrasonic Testing of Wrought Products, is the American practice. It applies to wrought metal products 6.35 mm (0.250 inch) thick or more, and it replaced the military standard MIL-STD-2154. It defines five acceptance classes, AAA, AA, A, B and C, in descending order of stringency. Each class is stated as a reference flat-bottomed hole size, with limits on loss of back reflection and noise and, for all but class C, on multiple and linear indications. ASTM A388 is the practice for ultrasonic examination of steel forgings, and some bar specifications cite it. Among the German steel industry's test sheets, SEP 1927 uses automated ultrasonic immersion testing of specimens taken from rolled or forged steel bars to determine their macroscopic cleanliness.
Quality classes and reference reflectors
The reference reflector in bar standards is the flat-bottomed hole: a hole drilled into a reference block of acoustically similar steel, with a flat end facing the probe. A natural discontinuity is reported by its equivalent flat-bottomed hole diameter, the diameter of the hole that would return an echo of the same amplitude at the same depth. The equivalent diameter measures reflectivity, not true size: an irregular or inclined inclusion reflects less sound than a flat disc of the same area.
EN 10308 sets a recording level and acceptance limits for each quality class. For ferritic and martensitic bars there are four classes. Class 1 records indications above an 8 mm equivalent flat-bottomed hole and class 4, the most stringent, records them above 2 mm; each class sets a tighter limit for extended or grouped indications than for isolated point indications, and a limit on the rapid loss of back-wall echo that a large reflector causes. A discontinuity is extended when its indication is longer than the beam width at its depth, and indications are grouped when their maxima lie 40 mm apart or less. Where the requirement differs across the section, the order names the zone to which each class applies.
Austenitic and austenitic-ferritic (duplex) stainless steel bars are treated separately. Their coarser and often directional grain structure scatters and attenuates sound, raising the background noise against which small echoes must be read. EN 10308 gives these steels three quality classes whose recording levels rise with bar thickness, so that a given class demands a smaller reflector in a thin bar than in a thick one. For coarse-grained austenitic material, ASTM A388 prefers a frequency of 1 MHz to its usual 2.25 MHz and allows 0.4 MHz where needed, trading resolution for penetration through the grain. Annealed austenitic grades are non-magnetic and duplex grades are magnetic, a difference set out in the article on whether stainless steel is magnetic, and one that matters more for eddy current testing than for ultrasound.
Eddy current testing: encircling coils and rotating probes
Eddy current testing applies an alternating current to an exciting coil placed close to the bar. The coil's alternating magnetic field induces circulating currents, eddy currents, in the surface of the bar, and these currents set up a field of their own that opposes the coil's field. A crack or seam interrupts the path of the eddy currents and changes the impedance of the coil or the voltage in a separate sensing coil. The instrument displays the change as a vector in the complex plane, and the phase of that vector helps separate defect signals from signals caused by changes in the gap between coil and bar.
Eddy currents are concentrated at the surface. Their density falls exponentially with depth, and the standard depth of penetration, at which the density has fallen to about 37 percent of its surface value, is inversely proportional to the square root of the product of frequency, electrical conductivity and magnetic permeability. A lower frequency therefore reaches deeper. Annealed austenitic stainless steel, of low conductivity and non-magnetic, allows deeper penetration than carbon or alloy steel at the same frequency. In ferromagnetic steels, ferritic, martensitic and duplex stainless grades among them, high and variable permeability confines the currents to a thin layer and produces false signals. A strong static magnetic field applied around the test coil saturates the steel, suppressing these permeability effects; ASTM E309 describes this magnetic saturation technique for steel tube.
Two coil arrangements are used on bar. An encircling coil surrounds the bar as it passes through and examines the whole circumference at once. A differential encircling coil compares two adjacent sections of the bar, so a defect that is continuous and uniform along the length, such as a long seam, can produce little or no signal; ASTM E309 records this limitation. Rotating probe systems spin small probe coils around the bar as it advances, so that each coil follows a helical path and crosses a longitudinal seam on every revolution. Eddy current testing is generally insensitive to defects close to the ends of the product, and ASTM E309 has the extent of this end effect determined on the reference standard.
Standards for eddy current testing of bar and tube
ISO 15549, Non-destructive testing: Eddy current testing: General principles, sets the framework for all eddy current examination of products, bars and wire rod among them, and gives guidance for the application documents that describe a particular product. It requires reference test pieces, normally of the same material and finished state as the product, carrying holes, notches or other known features; functional checks at least at the start and end of each examination; and personnel certified under ISO 9712 or equivalent. If a functional check fails, every product examined since the last successful check counts as untested.
The product standards for automated eddy current testing are written for tube. ISO 10893-2 covers seamless and welded steel tubes, other than submerged arc welded tubes, from 4 mm outside diameter, and was amended in 2020 to change the dimensions of its reference notch and its acceptance criteria. ASTM E309 covers ferromagnetic steel tube tested under magnetic saturation, and ASTM E426 covers tube of austenitic stainless steel, titanium and similar low-conductivity alloys. A bar test is defined by an application document or a written procedure of the kind ISO 15549 describes, agreed at the time of enquiry and order, which fixes the reference bar, the size and orientation of its notches or drilled holes, and the reject level. Signals from natural defects can differ from those of artificial notches, and ASTM E309 advises establishing the sensitivity needed to detect the natural defects that matter to the end use.
Ultrasonic and eddy current testing compared
| Feature | Ultrasonic testing | Eddy current testing |
|---|---|---|
| Physical principle | Reflection of high-frequency sound waves | Disturbance of induced electric currents |
| Region examined | Full volume, poorest just below the entry surface | Surface and near-surface layer |
| Typical defects found | Centre porosity, shrinkage, inclusion clusters, flakes, internal cracks | Seams, laps, slivers, surface cracks |
| Coupling | Water or another couplant between probe and bar | None, no contact with the bar |
| Reference reflector | Flat-bottomed holes in a reference block | Notches or drilled holes in a reference bar |
| Material effects | Coarse austenitic grain scatters sound and raises noise | Magnetic permeability of ferritic, martensitic and duplex steel needs saturation |
| Surface needed | Free from loose scale, paint and other matter that disturbs coupling | Free from scale, dirt and conductive residue |
| Governing documents | EN 10308, ASTM E2375, ASTM A388 | ISO 15549 (general principles); ISO 10893-2, ASTM E309 and E426 for tube |
Neither method replaces the other. A bar that passes an ultrasonic test may still carry a shallow seam that opens during machining or fatigue loading, and a bar that passes an eddy current test may still carry a centre defect that appears only when the part is bored. Shafting, valve stems and other parts that carry cyclic loads from the surface and are machined or bored through the centre may therefore be specified with both.
Ultrasonic and eddy current testing at Laxcon Steels
The inspection equipment of Laxcon Steels, listed on the quality page, includes an automatic ultrasonic testing machine for internal soundness and an automatic eddy current testing machine, which passes the bar through an encircling coil, for surface and near-surface defects. Every hot rolled round bar, from 16 to 125 mm, and every round cornered square bar is ultrasonically tested along its whole length, and proof machined bar, from 120 to 550 mm, is ultrasonically tested through its machined surface. Each precision shaft quality (PSQ) bar, from 8 to 81 mm, is ultrasonically checked, and PSQ and bright bar are eddy current tested when the order specifies it. The PSQ bar article sets out the tolerances and straightness of shaft bar.
Frequently asked questions
What is the difference between ultrasonic and eddy current testing of bar?
Ultrasonic testing sends sound into the bar and detects internal defects such as centre porosity, inclusion clusters and internal cracks through the full section. Eddy current testing induces electric currents in the surface and detects surface and near-surface defects such as seams, laps and cracks. Bar for shafts and other critical parts can be specified with both.
What is EN 10308?
EN 10308 is the European standard for ultrasonic testing of steel bars up to 400 mm in diameter or thickness. It describes pulse-echo testing with probes of 1 to 6 MHz, and it defines quality classes by the equivalent flat-bottomed hole size at which indications are recorded and accepted: four classes for ferritic and martensitic steels, and three thickness-dependent classes for austenitic and duplex stainless steels.
What does a flat-bottomed hole mean in ultrasonic testing?
A flat-bottomed hole is a drilled hole with a flat end, made in a reference block of similar steel, that serves as the standard reflector for setting test sensitivity. A defect is reported by the diameter of the flat-bottomed hole that would give an echo of the same amplitude at the same depth.
Why is eddy current testing of magnetic steel harder than of austenitic stainless steel?
The magnetic permeability of ferritic, martensitic and duplex steels confines eddy currents to a very thin surface layer and varies within the bar, producing signals unrelated to defects. Applying a strong magnetic field around the test coil saturates the steel and suppresses these effects. Annealed austenitic stainless steel is non-magnetic and normally needs no saturation.
Sources
- EN 10308:2001, Non-destructive testing: Ultrasonic testing of steel bars (BS EN 10308:2002): scope, probe frequency and types, couplant, stage of manufacture, surface condition, sensitivity setting, scanning, classification of discontinuities, quality classes and recording levels.
- ASTM E2375, Standard Practice for Ultrasonic Testing of Wrought Products.
- ASTM A388/A388M, Standard Practice for Ultrasonic Examination of Steel Forgings.
- SEP 1927, Ultrasonic immersion testing method for determining the macroscopic cleanliness rate of rolled or forged steel bars.
- ISO 15549:2019, Non-destructive testing: Eddy current testing: General principles.
- ISO 9712, Non-destructive testing: Qualification and certification of NDT personnel.
- ISO 10893-2, Non-destructive testing of steel tubes, Part 2: Automated eddy current testing of seamless and welded (except submerged arc-welded) steel tubes for the detection of imperfections.
- ASTM E309, Standard Practice for Eddy Current Examination of Steel Tubular Products Using Magnetic Saturation.
- ASTM E426, Standard Practice for Electromagnetic (Eddy Current) Examination of Seamless and Welded Tubular Products, Titanium, Austenitic Stainless Steel and Similar Alloys.