Solution Annealing of Stainless Steel: Temperature, Quenching and Corrosion Resistance
Send an enquirySolution annealing is a heat treatment that heats a stainless steel to a temperature at which its carbides and other secondary phases dissolve into the matrix, holds it there until the whole section has reached that temperature, and then cools it fast enough that the dissolved elements stay in solid solution at room temperature. The treatment is given to austenitic, duplex and precipitation hardening stainless steels. It restores the full corrosion resistance of the grade and removes the hardening left by cold work; in the austenitic and duplex grades it leaves the steel in its softest and most ductile condition. Product standards name the result as a delivery condition: Condition A in ASTM A276, the annealed condition in ASTM A479, and the symbol +AT in EN 10088-3. Ferritic and martensitic stainless steels are not solution annealed; they are annealed at lower temperatures, as described under soft annealing below.
What solution annealing changes
An austenitic stainless steel such as 304 holds its carbon in solid solution only at high temperature. At lower temperatures the equilibrium solubility of carbon in austenite falls below the carbon the grade contains, so a steel held for long enough at an intermediate temperature rejects carbon as chromium-rich M23C6 carbide. The carbide nucleates most easily on the grain boundaries. Each particle draws chromium from the metal immediately around it, and the narrow band beside the boundary can fall below the chromium content needed to keep a passive film. That band then corrodes preferentially in an acid or chloride medium while the grains themselves stay intact. This condition is called sensitisation.
Solution annealing reverses it. At the annealing temperature the carbides dissolve, chromium diffuses back into the depleted bands, and the composition across the grain becomes uniform again. The same temperature recrystallises a cold-worked structure: new, strain-free grains replace the deformed ones, and in 304 the strain-induced martensite formed by cold work reverts to austenite, which removes the weak magnetic response described in the article on whether stainless steel is magnetic.
In a duplex stainless steel the treatment has a further purpose. Duplex grades contain ferrite and austenite in roughly equal amounts, and between about 700 and 1,000 degrees Celsius their ferrite decomposes into sigma and other intermetallic phases that lower both toughness and corrosion resistance. The solution anneal dissolves those phases and fixes the ratio of the two structures; the ferrite fraction rises with the annealing temperature, so the anneal is held inside the grade's range rather than simply above a minimum. In a precipitation hardening grade such as 17-4 PH, the anneal takes copper into solution so that a later ageing treatment can precipitate it as a fine strengthening dispersion.
Annealing temperatures by grade
Each grade has its own temperature range. The lower limit is set by the temperature needed to dissolve the carbides or intermetallic phases of that composition, which rises with the chromium and molybdenum content. The upper limit is set by grain growth and, in duplex grades, by the ferrite fraction. The guideline values compiled for the grades of EN 10088 are summarised below.
| Grade | EN number | Range, degrees Celsius | Cooling |
|---|---|---|---|
| 304, 304L | 1.4301, 1.4307 | 1,000 to 1,100 | Water or air |
| 321 | 1.4541 | 1,000 to 1,100 | Water or air |
| 316, 316L | 1.4401, 1.4404 | 1,030 to 1,110 | Water or air |
| 316Ti | 1.4571 | 1,030 to 1,110 | Water or air |
| 904L | 1.4539 | 1,060 to 1,140 | Water or air |
| 2304 | 1.4362 | 950 to 1,050 | Water or air |
| 2205 | 1.4462 | 1,020 to 1,100 | Water or air |
| 2507 | 1.4410 | 1,040 to 1,120 | Water or air |
| 17-4 PH | 1.4542 | 1,025 to 1,055 | Air |
304, 304L, 316 and 316L are austenitic grades, 321 and 316Ti austenitic grades stabilised with titanium, and 904L a high-alloy austenitic grade; 2304 and 2205 are duplex, 2507 super duplex and 17-4 PH a precipitation hardening grade. The cooling of 304, 304L, 316 and 316L must be fast enough to avoid sensitisation, and that of 2205 fast enough to avoid precipitation.
Ranges published by producers and American sources differ from these by up to a few tens of degrees. One American producer gives 1,038 to 1,121 degrees Celsius for 304, and the International Molybdenum Association gives a minimum of 1,040 degrees Celsius for UNS S32205, above the European lower limit for the equivalent 1.4462. ASTM A564 sets Condition A of type 630, the American designation of 17-4 PH, at 1,040 degrees Celsius plus or minus 15 degrees, the same band as the European guideline for 1.4542. The purchase specification names the standard whose range applies. When the treatment is carried out in a continuous furnace, the upper part of the range is usually preferred, or even exceeded.
Cooling and the sensitisation range
The cooling rate decides whether the anneal succeeds. Chromium carbide forms in austenitic stainless steel over a band of temperature that published sources place between about 425 and 850 degrees Celsius, and the precipitation is fastest at an intermediate temperature within it: carbides can appear on the grain boundaries after only a few minutes near 750 degrees Celsius. A slow cool through the band re-precipitates the carbides the anneal dissolved. The rate needed falls with the carbon content, so the L grades, with 0.03 percent carbon maximum, tolerate a slower cool than the standard grades, as the 304 against 304L and 316 against 316L article sets out.
The section thickness then decides the medium. Thin strip and wire lose heat to the air quickly enough to pass the band in time. The guideline tables for the grades of EN 10088 list air or water for the austenitic grades, on the condition that the cooling is fast enough to avoid intergranular corrosion. A bar of large diameter cools far more slowly at its centre, and heavy sections are quenched in water. The result, not the medium, is what counts: the measure is freedom from susceptibility to intergranular corrosion, as tested to EN ISO 3651-2 or ASTM A262. In ASTM A262, Practice A is an electrolytic etch in oxalic acid, examined under the microscope, and Practice E exposes a specimen to copper and copper sulphate in sulphuric acid and then bends it to look for fissures; the ASTM A262 intergranular corrosion tests article describes each practice.
Duplex grades are cooled under a stricter rule. The guidance of the International Molybdenum Association is that a duplex part should be water quenched from the annealing temperature and should not spend several minutes between 700 and 1,000 degrees Celsius while it is moved from the furnace to the quench. A precipitation hardening grade is cooled differently again. ASTM A564 requires Condition A of type 630 to be cooled to below 32 degrees Celsius, so that the austenite present at the annealing temperature has completed its transformation to martensite before the steel is aged.
Solution annealing, stress relieving and soft annealing
Three treatments with similar names use different temperatures and produce different conditions. The temperatures in the table are typical values. Solution annealing is followed by rapid cooling in water or air, low-temperature stress relief by cooling in air, and soft annealing by the cooling its grade requires.
| Treatment | Grades | Degrees Celsius | Effect |
|---|---|---|---|
| Solution annealing | Austenitic, duplex, precipitation hardening | About 950 to 1,140, by grade | Carbides and intermetallics dissolved, cold work removed, full corrosion resistance |
| Low-temperature stress relief | Austenitic | About 400 | Part of the residual stress relieved; structure, strength and corrosion resistance unchanged |
| Soft annealing | Ferritic, martensitic | About 745 to 830 for 410, 420 and 430 | Softened for machining or forming; the +A condition of EN 10088-3 |
Stress relieving reduces the residual stress left by machining, forming or welding without changing the structure. In austenitic grades a treatment near 400 degrees Celsius sits below the sensitisation range and gives partial relief; one producer of 304 recommends 399 degrees Celsius for half an hour to two hours for cold-worked parts. A stress relief at a higher temperature passes into the sensitisation range, so it is applied to the L and stabilised grades rather than to the standard carbon grades. A full solution anneal relieves the old stresses, but its rapid cool creates new ones of considerable magnitude. Duplex grades have no satisfactory stress relieving temperature: no temperature below the solution annealing range relieves stress in them without the risk of intermetallic phases, so a duplex part that must be relieved of stress is given a full solution anneal and water quench instead.
Soft annealing is the anneal of the ferritic and martensitic grades, among them 430, 410 and 420. Their guideline annealing temperatures lie between about 745 and 830 degrees Celsius, well below the temperatures from which the martensitic grades are hardened. It leaves ferrite and spheroidised carbide, a structure that machines well, and in a martensitic grade it is the condition from which the steel is later hardened and tempered, as the heat treatment of steel article describes.
The annealed condition in bar standards
Bar standards state the solution annealed condition as a requirement. ASTM A276, the general specification for stainless steel bars, names five conditions: A, annealed; H and T, hardened and tempered at a lower and a higher temperature; S, strain hardened by light cold work; and B, severely cold worked. ASTM A479, the bar specification for boiler and pressure vessel construction, requires its austenitic grades to be heat treated and corrosion tested. The ASTM A276 and A479 article compares the two. EN 10088-3 writes the condition as a symbol after the grade: +AT, solution annealed, for the austenitic and duplex grades and for the precipitation hardening grades before ageing, and +A, annealed, for the ferritic and martensitic grades, as the EN 10088-3 and EN 10278 article explains.
Precipitation hardening bar is supplied in Condition A of ASTM A564 or aged to an H condition. Condition A is the machining condition, and in critical applications the steel is aged before service, because ageing, particularly at the higher ageing temperatures, gives more reliable resistance to stress corrosion cracking than the unaged steel. ISO 15156-3, the corrosion-resistant alloy part of NACE MR0175 / ISO 15156, accepts the common austenitic grades in the solution annealed condition, free of cold work intended to raise their strength, as set out in the NACE MR0175 / ISO 15156 article.
Annealing after welding and cold work
A fusion weld heats the parent metal beside it to every temperature from the melting point down to ambient. In a straight-carbon grade, 304 or 316, the band that spent its share of the cycle inside the sensitisation range can sensitise. Most austenitic weldments are nevertheless used as welded: the L and stabilised grades avoid the problem, and modern standards have removed many of the post-weld stress relief requirements once applied to these steels. Post-weld solution annealing is given mainly in two cases: heavy welded sections in a standard carbon grade that are destined for a medium attacking sensitised metal, and duplex welds, particularly those made without filler metal, that must regain the phase balance and corrosion resistance of the parent metal. In both cases the whole part goes into the furnace and is quenched. Heating the weld alone would leave a band at the edge of the heated zone that had itself been held inside the sensitisation range.
Cold work raises strength and hardness and lowers elongation. Some designs use that strength on purpose: ASTM A276 Conditions S and B and the strain-hardened 316 of ASTM A479 are delivered cold worked. Others need the annealed properties, and the bar or part is solution annealed after the last forming step. Heavily formed austenitic parts are also annealed between forming stages when the steel has hardened too far to deform further without cracking. For duplex steel the International Molybdenum Association gives a conservative rule for a repeat anneal: the hold at temperature should be comparable to the total time the part has spent between 650 and 980 degrees Celsius since its previous full anneal.
Scale and pickling after annealing
An anneal in air grows a scale rich in chromium oxide, and the metal immediately beneath it loses chromium to the scale. The surface then resists corrosion less well than the bulk, and it is restored by removing both layers, usually by pickling in a mixture of nitric and hydrofluoric acids, as ASTM A380 describes, or by grinding, peeling or blasting followed by passivation. The passivation and pickling article describes the chemistry. EN 10088-3 records the surface finish of a bar with its own codes, so that a bar heat treated and pickled after hot rolling carries the finish 1D.
Bright annealing avoids the scale. The steel is heated and cooled in a reducing or inert atmosphere, typically hydrogen, dissociated ammonia or argon, and leaves the furnace without oxide. In either method the steel is cleaned before it enters the furnace, because oil, grease and marking residues burnt into the surface at the annealing temperature can add carbon to the metal beneath them.
Solution annealing at Laxcon Steels
The heat treatment department of Laxcon Steels includes three gas-fired, PLC-controlled solution annealing furnaces of 6 MT each and a 60 KL water quenching tank, with a 40 MT soft annealing furnace, two electric tempering furnaces of 10 MT and 18 MT, and a furnace built for bars up to 7 metres long, as listed on the technology page. Solution annealing is one of the heat treatments listed for hot rolled round bars from 16 to 125 mm and for bright bars from 5 to 115 mm. Precipitation hardening steels in 17-4 PH and 15-5 PH are offered in the solution annealed condition and in the aged conditions from H900 to H1150M. The austenitic, duplex and precipitation hardening grades are listed in the grade reference.
Frequently asked questions
What is the solution annealing temperature of 304 stainless steel?
The EN 10088 guideline range for 1.4301, the European equivalent of 304, is 1,000 to 1,100 degrees Celsius; an American producer gives 1,038 to 1,121 degrees Celsius. The bar is held until its centre reaches the temperature and is then cooled rapidly, in water for heavy sections.
Why is stainless steel quenched after solution annealing?
Chromium carbide re-forms at the grain boundaries if the steel cools slowly through the sensitisation range, roughly 425 to 850 degrees Celsius. Cooling quickly carries the steel through that band in too short a time for the carbide to nucleate, so the steel keeps the corrosion resistance the anneal restored. In duplex grades the quench prevents sigma phase in the same way.
Is solution annealing the same as stress relieving?
No. Solution annealing heats an austenitic stainless steel above about 1,000 degrees Celsius to dissolve carbides and remove cold work, and it ends with a rapid cool. Stress relieving uses a much lower temperature, about 400 degrees Celsius for austenitic grades, and reduces residual stress without changing the structure. Duplex grades have no safe stress relieving temperature and are solution annealed instead.
Does a welded stainless steel part need solution annealing?
Usually not. Most austenitic weldments are used as welded, and the low-carbon L grades and the titanium- and niobium-stabilised grades 321 and 347 resist sensitisation in an ordinary welding cycle. A post-weld solution anneal of the whole part is given where a standard carbon grade has been welded in a heavy section for corrosive service, or where a duplex weld must regain the properties of the parent metal.
Sources
- ASTM A276/A276M, Standard Specification for Stainless Steel Bars and Shapes: Conditions A, H, T, S and B.
- ASTM A479/A479M, Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels: heat treatment and corrosion testing of the austenitic grades.
- ASTM A564/A564M, Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes: Condition A of type 630.
- ASTM A262, Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels.
- ASTM A380/A380M, Standard Practice for Cleaning, Descaling, and Passivation of Stainless Steel Parts, Equipment, and Systems.
- EN 10088-3, Stainless steels, Part 3: technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products: heat treatment condition symbols and surface finishes.
- EN ISO 3651-2, Determination of resistance to intergranular corrosion of stainless steels, Part 2: ferritic, austenitic and ferritic-austenitic (duplex) stainless steels, corrosion test in media containing sulfuric acid.
- ISO 15156-3, Petroleum and natural gas industries, Materials for use in H2S-containing environments in oil and gas production, Part 3: cracking-resistant CRAs (corrosion-resistant alloys) and other alloys.
- Euro Inox, Stainless Steels: Tables of Fabrication Parameters, Materials and Applications Series, Volume 17: guideline heat treatment temperatures for the grades of EN 10088.
- International Molybdenum Association, Practical Guidelines for the Fabrication of Duplex Stainless Steels, second edition, 2009: solution annealing, quenching and stress relief of duplex grades.