title: "Hardness Testing: Brinell, Rockwell and Vickers Methods"
source: "https://www.laxconsteels.com/hardness-testing-brinell-rockwell-vickers/"
description: "The Brinell, Rockwell and Vickers hardness tests explained: ISO 6506-1, 6508-1 and 6507-1, indenters, forces, scales, test conditions and conversion limits."
---
# Hardness Testing of Metals: The Brinell, Rockwell and Vickers Methods and How the Scales Convert

Send an enquiry

9 min read

A hardness test is a mechanical test that measures the resistance of a metal to permanent indentation. An indenter of defined shape is pressed into the surface under a defined force, and the size or depth of the impression it leaves is converted into a hardness number. The Brinell test presses a tungsten carbide ball and measures the diameter of the impression. The Rockwell test measures the depth to which a diamond cone or a ball penetrates. The Vickers test presses a square diamond pyramid and measures the diagonals of the impression. The three are defined internationally by ISO 6506-1, ISO 6508-1 and ISO 6507-1, and in North America by ASTM E10, ASTM E18 and ASTM E92. A hardness number has meaning only together with the method, indenter and force that produced it, which is why every result carries a symbol such as HBW, HRC or HV.

## Indentation hardness and what it measures

An indenter loaded against a metal surface first deforms the metal elastically and then makes it flow plastically outward and upward. When the force is removed, the elastic part recovers and a permanent impression remains. The smaller or shallower that impression under a given force, the harder the metal. Indentation hardness is therefore not a single physical constant. It combines the yield strength of the metal, its strain hardening around the indenter and, for the methods that measure depth, its elastic recovery. It differs from scratch hardness and from rebound hardness, which measures how fast a body fired at the surface bounces back.

## The Brinell test: ISO 6506-1 and ASTM E10

The Brinell test presses a polished tungsten carbide ball into the surface, holds the force, removes it, and measures the diameter of the round impression in two directions at right angles. The hardness is the test force, in kilogram-force equivalents, divided by the curved area of the impression. ISO 6506-1:2014 admits balls of 10, 5, 2.5 and 1 mm and forces from 9.807 newtons to 29.42 kilonewtons. The classic condition for steel is the 10 mm ball under 29.42 kilonewtons, traditionally written 3,000 kgf.

A ball impression changes shape as it deepens, so Brinell results are comparable only at the same ratio of force to the square of the ball diameter. ISO 6506-1 calls this the force-diameter index and recommends 30 for steel, nickel alloys and titanium alloys. The force is chosen so that the impression diameter lies between 0.24 and 0.6 times the ball diameter. It is applied over 2 to 8 seconds and held for 10 to 15 seconds. The result is rounded to three significant figures and written with the ball and the force, as in 229 HBW 10/3000. The W marks the tungsten carbide ball; the hardened steel ball of earlier editions, written HB or HBS, has been withdrawn. Some product standards, ASTM A564 among them, still write the symbol HB.

The 10 mm ball leaves an impression several millimetres wide, which samples many grains and smooths out segregation, so Brinell suits castings, rolled sections and annealed or hardened and tempered bar. Tungsten carbide deforms measurably on very hard steel, so the test is not used above about 650 HBW, and the impression is too large for thin sections and finished surfaces.

## The Rockwell test: ISO 6508-1 and ASTM E18

The Rockwell test measures depth instead of area. A preliminary force seats the indenter and sets a reference level below surface roughness. An additional force is applied and removed, and the machine measures the permanent increase in depth while the preliminary force still acts. The number is read directly, with no optical measurement, so the test takes seconds. Each unit is a fixed depth: 0.002 mm on the regular scales and 0.001 mm on the superficial scales. The depth in units is subtracted from 100 on the diamond scales and the superficial ball scales, or from 130 on the regular ball scales, so a harder metal gives a higher number.

ISO 6508-1:2023 defines nine regular and six superficial scales. On the regular scales the preliminary force is 98.07 newtons (10 kgf) and the total force 60, 100 or 150 kgf. The C scale (HRC) uses a diamond cone with a 120 degree angle and a 0.2 mm tip radius under 150 kgf, and applies from 20 to 70 HRC, the range of hardened and precipitation hardened steels. The B scale (HRBW) uses a 1.5875 mm (one-sixteenth inch) tungsten carbide ball under 100 kgf and covers softer metals, such as annealed carbon and austenitic stainless steel, up to 100 HRBW. The A scale (HRA) uses the diamond cone under 60 kgf, for cemented carbides and for hardened parts too thin for the C scale. The superficial N scales (diamond) and T scales (ball) use a preliminary force of 3 kgf and totals of 15, 30 or 45 kgf, for thin sheet, strip and hardened surfaces. Results on different Rockwell scales cannot be compared directly, because each scale is its own combination of indenter and force.

## The Vickers test: ISO 6507-1, ASTM E92 and ASTM E384

The Vickers test presses a square-based diamond pyramid, with 136 degrees between opposite faces, into the surface and measures both diagonals of the impression under a microscope. The hardness is the force divided by the sloping area of the impression: 0.1891 times the force in newtons divided by the square of the mean diagonal in millimetres. The force is applied over 2 to 8 seconds and held for 10 to 15 seconds, and the result is written with the force in kilogram-force equivalents, as in 640 HV 30.

A pyramid impression keeps the same shape at any depth, so in principle the Vickers number does not depend on the force. The same scale therefore serves annealed copper and hardened tool steel, including steels too hard for the Brinell ball. ISO 6507-1 divides the test into three ranges: the Vickers test at 49.03 newtons (HV 5) and above, the low-force test from HV 0.2 to below HV 5, and the microhardness test from HV 0.01 to below HV 0.2. ASTM E384 covers microindentation from 1 to 1,000 gram-force. At these forces the test measures single phases, coatings, decarburised layers, weld zones and, as a row of impressions inward from the surface, the depth of a hardened case, as described in the [case hardening](https://www.laxconsteels.com/case-hardening-of-steel/) article.

## The Knoop test and portable methods

The Knoop test, defined by ISO 4545-1 and by ASTM E92 and E384, uses an elongated rhombic diamond pyramid whose long diagonal is about seven times its short one. Only the long diagonal is measured. The impression is much shallower than a Vickers impression of the same length, which suits thin layers and brittle materials. Knoop numbers vary with force, particularly below 200 gram-force, so results are compared only at the same force.

The Leeb test, defined by ISO 16859-1 and, for steel and cast iron, by ASTM A956, fires an impact body with a hard spherical tip at the surface and measures its velocity before and after impact. The Leeb number is the ratio of rebound velocity to impact velocity multiplied by 1,000, written with the impact device, as in HLD. The rebound depends on elastic as well as plastic behaviour, so a Leeb value converts to a static scale only through tables for that material. The ultrasonic contact impedance (UCI) method of ASTM A1038 presses a Vickers diamond mounted on a rod vibrating at an ultrasonic frequency. The frequency shifts by an amount that grows with the contact area, and the instrument converts the shift to a Vickers or Rockwell value through a calibration that depends on the material.

## The methods compared

*Hardness test methods for metals compared: indenter, force, quantity measured and notation*

| Method | Indenter | Force | Measured | Notation |
| --- | --- | --- | --- | --- |
| Brinell | Tungsten carbide ball, 1 to 10 mm | 9.807 N to 29.42 kN | Impression diameter | 229 HBW 10/3000 |
| Rockwell, regular | Diamond cone or ball | 10 kgf preliminary; 60, 100 or 150 kgf total | Permanent depth | 45 HRC, 85 HRBW |
| Rockwell, superficial | Diamond cone or 1.5875 mm ball | 3 kgf preliminary; 15, 30 or 45 kgf total | Permanent depth | 70 HR30N, 70 HR30TW |
| Vickers | Square diamond pyramid, 136 degrees | From 0.09807 N, in three ranges | Both diagonals | 640 HV 30 |
| Knoop | Elongated rhombic diamond pyramid | Up to about 19.6 N | Long diagonal | HK with the force |
| Leeb rebound | Impact body with a hard spherical tip | Impact | Rebound and impact velocity | HLD |
| Ultrasonic contact impedance | Vickers diamond on a vibrating rod | Set by the probe | Shift in resonant frequency | Converted to HV or HRC |

The methods are standardised in ISO 6506-1 and ASTM E10 for Brinell; ISO 6508-1 and ASTM E18 for Rockwell, regular and superficial; ISO 6507-1, ASTM E92 and ASTM E384 for Vickers; ISO 4545-1, ASTM E92 and ASTM E384 for Knoop; ISO 16859-1 and ASTM A956 for Leeb rebound; and ASTM A1038 for ultrasonic contact impedance.

Indian Standards adopt the ISO methods as IS 1500 (Part 1) for Brinell, IS 1586 (Part 1) for Rockwell and IS 1501 (Part 1) for Vickers.

## Surface, thickness, spacing and curved surfaces

Every method assumes a smooth, even surface, free from oxide scale, foreign matter and lubricant, and prepared so that heating or cold working alters the surface as little as possible. A hot rolled or heat-treated bar carries scale and may carry a softer decarburised skin, so it is ground or machined back before testing. The test piece must be thick enough that the indenter does not feel the support: at least eight times the impression depth for Brinell under ISO 6506-1, ten times the permanent depth for the Rockwell diamond scales and fifteen times for the ball scales under ISO 6508-1, and one and a half times the mean diagonal for Vickers under ISO 6507-1. For Brinell, and for Vickers on steel, each impression centre lies at least two and a half impression widths from the edge and three from the next centre, outside the work-hardened zone of its neighbour.

A Rockwell reading on the curved surface of a round bar is lower than the true hardness, because the metal beside the indenter falls away and gives less support. The error grows as the diameter falls. ISO 6508-1 and ASTM E18 tabulate corrections to be added for convex cylindrical surfaces, and ISO 6508-1 adds corrections for spherical surfaces on the C scale. A flat ground on the bar, or a test on a cross-section, avoids them. The Brinell and Rockwell standards call, in general, for a test temperature of 10 to 35 degrees Celsius.

## Conversion between scales: ASTM E140 and ISO 18265

No exact relationship links the scales. The methods strain the metal to different degrees, measure area or depth, and respond differently to elastic recovery and work hardening. Conversion tables are therefore empirical, compiled from paired tests on one family of material and valid only for it. ASTM E140 has separate tables for non-austenitic steels, nickel alloys, austenitic stainless steel plate and sheet, cartridge brass, copper, alloyed white iron and wrought aluminium, and a table for Leeb D values on non-austenitic steel. ISO 18265:2013 covers unalloyed and low-alloy steels, cast steel, tool steels, high-speed steels, hardmetals and non-ferrous metals.

Both standards treat a converted value as an approximation. ASTM E140 states that confidence limits for a conversion cannot be given, and ISO 18265 that a converted value is not a replacement for a value obtained by the correct standard method. ISO 6506-1 requires a test report to state the basis and method of any conversion. Approximate equivalents for non-austenitic steel are tabulated in the [hardness conversion chart](https://www.laxconsteels.com/hardest-metals/#conversion-chart) of the hardest metals article.

## Hardness and tensile strength

Indentation hardness and tensile strength both measure resistance to plastic flow, and in steel they rise together. Plasticity theory explains the link. The metal under an indenter is confined by the material around it, so the mean pressure needed to drive the indenter is about three times the flow stress. Hardness therefore tracks tensile strength well enough to check a heat treatment or a batch. The link varies with strain-hardening behaviour: ISO 18265 calls its tensile values the least reliable of its conversions, and ISO 6506-1 notes that no general method converts Brinell hardness accurately into tensile strength. Hardness does not replace the tensile test a product standard requires, which also reports proof stress and elongation, as set out in the [yield strength and tensile strength](https://www.laxconsteels.com/yield-strength-vs-tensile-strength/) article.

## Hardness in product standards and service codes

Product standards state hardness as a maximum, a minimum or a range on a named scale. A maximum keeps a softened bar machinable; a minimum confirms that a hardening treatment has worked. ASTM A564 sets a maximum of 363 HB for [17-4PH](https://www.laxconsteels.com/grades/17-4-ph/) bar in the solution treated Condition A and a minimum of 388 HB after ageing at H900; the other conditions are tabulated on the [precipitation hardening steels](https://www.laxconsteels.com/products/precipitation-hardening-steels/) page. Values for each stainless family in its delivery conditions are in the [hardness of stainless steel by grade](https://www.laxconsteels.com/hardness-of-stainless-steel-by-grade/) article.

Service codes use hardness to limit susceptibility to cracking. ISO 15156-2, for carbon and low-alloy steel in oil and gas production containing hydrogen sulphide, sets a general limit of 22 HRC and states its weld limits in Vickers units, since hardness changes within a few millimetres across a weld; the [NACE MR0175 and ISO 15156](https://www.laxconsteels.com/nace-mr0175-iso-15156-norsok-m-650/) article describes those limits. The Jominy end-quench test of ISO 642 and ASTM A255 quenches one end of a bar and records hardness along it, which measures hardenability, the property described in the [heat treatment of steel](https://www.laxconsteels.com/heat-treatment-of-steel/) article.

## Mechanical testing at Laxcon Steels

The Laxcon Steels laboratory at Sanand holds NABL accreditation to ISO/IEC 17025:2017 in the field of testing, certificate TC-12337. Its mechanical testing bench, impact tester and metallography equipment are shown on the [quality](https://www.laxconsteels.com/quality/) page. Laxcon Steels supplies [hot rolled round bar](https://www.laxconsteels.com/products/hot-rolled-round-bars/) from 16 to 125 mm, and 17-4PH bar either solution treated in Condition A or aged to the condition ordered.

## Frequently asked questions

### What is the difference between the Brinell, Rockwell and Vickers hardness tests?

Brinell presses a tungsten carbide ball and measures the diameter of the impression. Rockwell presses a diamond cone or a ball and measures the permanent depth, reading the number directly. Vickers presses a square diamond pyramid and measures the diagonals. Brinell averages over coarse structures, Rockwell is the quickest, and Vickers covers the widest range, down to microscopic impressions.

### What does HRC mean?

HRC is hardness on the Rockwell C scale: a diamond cone under a total force of 150 kgf, each unit equal to 0.002 mm of permanent depth. It is used from 20 to 70 HRC for hardened steels. Softer metals are tested on the ball-based B scale.

### Which hardness test is used for thin material and surface layers?

Thin sheet, strip and small parts are tested on the Rockwell superficial scales or by the low-force Vickers test. Coatings, case depths, weld zones and single phases are measured by Vickers or Knoop microhardness on a polished cross-section.

### Can Vickers or Brinell hardness be converted exactly to Rockwell C?

No. Conversions are empirical and approximate, and ASTM E140 and ISO 18265 give separate tables for each family of material. ISO 18265 states that a converted value is not a replacement for a value obtained by the correct standard method.

## Sources

- ISO 6506-1:2014, Metallic materials, Brinell hardness test, Part 1: test method.
- ISO 6508-1:2023, Metallic materials, Rockwell hardness test, Part 1: test method.
- ISO 6507-1:2023, Metallic materials, Vickers hardness test, Part 1: test method.
- ISO 4545-1:2023, Metallic materials, Knoop hardness test, Part 1: test method.
- ISO 16859-1, Metallic materials, Leeb hardness test, Part 1: test method.
- ISO 18265:2013, Metallic materials, conversion of hardness values.
- ASTM E10, Standard Test Method for Brinell Hardness of Metallic Materials.
- ASTM E18, Standard Test Methods for Rockwell Hardness of Metallic Materials.
- ASTM E92, Standard Test Methods for Vickers Hardness and Knoop Hardness of Metallic Materials.
- ASTM E384, Standard Test Method for Microindentation Hardness of Materials.
- ASTM E140, Standard Hardness Conversion Tables for Metals.
- ASTM A956/A956M, Standard Test Method for Leeb Hardness Testing of Steel Products.
- ASTM A1038, Standard Test Method for Portable Hardness Testing by the Ultrasonic Contact Impedance Method.
- ASTM A564/A564M, Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes.
- ISO 15156-2, Petroleum and natural gas industries, materials for use in H2S-containing environments in oil and gas production, Part 2: cracking-resistant carbon and low-alloy steels.
- IS 1500 (Part 1), IS 1586 (Part 1) and IS 1501 (Part 1), the Indian adoptions of ISO 6506-1, ISO 6508-1 and ISO 6507-1.
- D. Tabor, The Hardness of Metals, Oxford University Press, 1951.

![Stainless steel hot rolled round bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-hot-rolled-round-bars.webp)

Enquire about **Hot Rolled Round Bars**

First name Last name Email Phone Company Location

Product

- Bright Bars
- Precision Shaft Quality (PSQ) Bars
- Pipes and Tubes
- Hexagonal Bright Bars
- Square Bright Bars
- Cold-Drawn Flat Bars
- Forged & Proof Machined Bars
- HRAP Flat Bars
- HRAP Equal Angles
- HRAP Unequal Angles
- Threaded Bars
- Hot Rolled Round Cornered Squares (RCS) Bars
- Hot Rolled Round Bars
- Continuous Cast Billets / Blooms
- Channels
- Forging Quality Ingots
- Precipitation Hardening Steels
- Duplex Steel
- T-Profile
- Others

Message

\* Required

## From the Mill

- [![Stainless steel hot rolled round bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-hot-rolled-round-bars.webp) Hot Rolled Round Bars 16 mm to 125 mm](https://www.laxconsteels.com/products/hot-rolled-round-bars/)
- [![Precipitation hardening stainless steel bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-precipitation-hardening-bars.webp) Precipitation Hardening Steels](https://www.laxconsteels.com/products/precipitation-hardening-steels/)
- [![Optical emission spectrometer used to certify grade composition](https://www.laxconsteels.com/images/quality/laxcon-steels-optical-emission-spectrometer.webp) Grade reference](https://www.laxconsteels.com/grades/)