title: "Hardness of Stainless Steel by Grade and Condition"
source: "https://www.laxconsteels.com/hardness-of-stainless-steel-by-grade/"
description: "Hardness of stainless steel by grade and condition: 304, 316, 430, 410, 420, 431, 440C, duplex 2205 and 17-4 PH, with the standards and sour-service limits."
---
# Hardness of Stainless Steel by Grade and Condition: Austenitic, Ferritic, Martensitic, Duplex and Precipitation Hardening

Send an enquiry

10 min read

The hardness of stainless steel is its resistance to permanent indentation, reported as a number on the Brinell (HB), Rockwell (HRB or HRC) or Vickers (HV) scale. It is not a fixed property of a grade. Two factors set it. The first is the metallurgical family, which decides whether the steel can be hardened by heat treatment at all. The second is the condition of the bar: annealed, cold worked, quenched and tempered, or aged. EN 10088-3 gives annealed austenitic and ferritic bar guidance maxima of about 200 to 230 HB. The response-test minimums of the hardenable martensitic grades run from 35 HRC for 410 to 58 HRC for 440C. The aged conditions of the precipitation hardening grade 17-4 PH, from H1150 to H900, require minimums of 28 to 40 HRC. A hardness figure therefore has meaning only together with its condition, its scale and the standard that sets it.

## Why hardness depends on family and condition

The five families of stainless steel differ in crystal structure, which decides how each responds to heat. Austenitic grades such as 304 and 316 stay face-centred cubic on quenching, and ferritic grades such as 430 stay body-centred cubic; neither can be hardened by heat treatment, and only cold work raises their hardness. Martensitic grades such as 410, 420 and 440C transform to martensite when quenched from the hardening temperature. Their carbon content sets the hardness the martensite reaches, and tempering trades part of it for toughness. Duplex grades such as 2205 are solution annealed and have no hardening treatment. Precipitation hardening grades such as 17-4 PH are solution treated, then held at a low ageing temperature that precipitates fine copper-rich particles and raises hardness without a quench.

Standards treat hardness in two ways. Where ASTM A276, A564 and A582 give a hardness value, it is a requirement that the bar must meet. In EN 10088-3 the hardness columns of the mechanical property tables are marked as guidance only, and the tensile properties are the binding values. Soft austenitic and ferritic material is usually tested on the Brinell or Rockwell B scale, and hardened martensitic and precipitation hardening material on the Rockwell C scale. The indentation methods themselves, and the limits of converting one scale into another under ISO 18265 and ASTM E140, are described in [hardness testing: Brinell, Rockwell and Vickers](https://www.laxconsteels.com/hardness-testing-brinell-rockwell-vickers/).

## Hardness of common stainless grades by condition

A maximum applies to a soft supply condition; a minimum applies to an aged condition or to the response test that proves a martensitic bar can harden. The first table gives the maxima and the second the minima. The grades are austenitic (304 and 316), ferritic (430), martensitic (410, 420, 431 and 440C), duplex (2205), super duplex (2507) and precipitation hardening (17-4 PH). The EN 10088-3 values are given for guidance.

*Maximum hardness of common stainless steel grades in the soft supply condition, with the condition and the standard that sets each limit*

| Grade | Hardness, max | Condition and standard |
| --- | --- | --- |
| 304 (1.4301) | 215 HB | Solution annealed bar to 160 mm; EN 10088-3 |
| 316 (1.4401) | 215 HB | Solution annealed bar to 160 mm; EN 10088-3 |
| 304 | 201 HB or 92 HRB | Annealed plate, sheet and strip; ASTM A240 |
| 316 | 217 HB or 95 HRB | Annealed plate, sheet and strip; ASTM A240 |
| 304 (B8) | 223 HB or 96 HRB | Bolting, Class 1, carbide solution treated; ASTM A193 |
| 304 (B8) | 321 HB or 35 HRC | Bolting, Class 2, solution treated and strain hardened; ASTM A193 |
| 430 (1.4016) | 200 HB | Annealed bar to 100 mm; EN 10088-3 |
| 410 (1.4006) | 220 HB | Annealed bar; EN 10088-3 |
| 420 (1.4021) | 241 HB | Annealed, hot finished; ASTM A276 |
| 431 (1.4057) | 285 HB | Annealed; ASTM A276 |
| 440C | 269 HB | Annealed, hot finished; ASTM A276 |
| 2205 (1.4462) | 270 HB | Solution annealed bar to 160 mm; EN 10088-3 |
| 2507 (1.4410) | 290 HB | Solution annealed bar to 160 mm; EN 10088-3 |
| 17-4 PH | 363 HB or 38 HRC | Condition A, solution treated; ASTM A564 |

*Minimum hardness of martensitic and precipitation hardening stainless steel grades after hardening or ageing, with the condition and the standard that sets each limit*

| Grade | Hardness, min | Condition and standard |
| --- | --- | --- |
| 410 | 35 HRC | Response to heat treatment; ASTM A276 |
| 420 | 50 HRC | Response to heat treatment; ASTM A276 |
| 431 | 40 HRC | Response to heat treatment; ASTM A276 |
| 440C | 58 HRC | Response to heat treatment; ASTM A276 |
| 17-4 PH | 388 HB or 40 HRC | H900; ASTM A564 |
| 17-4 PH | 277 HB or 28 HRC | H1150; ASTM A564 |

## Austenitic grades: annealed hardness and cold work

EN 10088-3 gives 215 HB as the guidance maximum for solution annealed [304](https://www.laxconsteels.com/grades/aisi-304/) (1.4301), 304L (1.4307), [316](https://www.laxconsteels.com/grades/aisi-316/) (1.4401) and 316L (1.4404) bar up to 160 mm, and 230 HB for the nitrogen-alloyed 304LN (1.4311). The figures most often quoted for 304 and 316, 201 HB or 92 HRB and 217 HB or 95 HRB, come from ASTM A240. That standard covers plate, sheet and strip, so its limits describe flat products, not bar. The higher figure for 316 reflects the solid-solution strengthening of molybdenum.

Cold work is the only route to higher hardness in this family, and austenite work hardens rapidly. EN 10088-3 allows the annealed hardness maximum to rise by 100 HB, or the tensile strength by 200 MPa, for bars up to 35 mm thick finished by a final cold deformation. For bar deliberately cold worked to strength, the standard specifies tensile levels rather than hardness: the +C700 and +C800 levels of the cold work hardened condition, for diameters agreed at order and normally not above 35 mm and 25 mm respectively. ASTM A193 expresses the same effect as hardness limits for bolting. Grade B8 in Class 1, carbide solution treated, is held to 223 HB, while Class 2, strain hardened after solution treatment, is allowed up to 321 HB or 35 HRC. A solution anneal returns cold-worked bar to its annealed hardness.

## Ferritic grades

Ferritic stainless steels have a narrow hardness range because neither quenching nor ageing hardens them, and they work harden more slowly than austenitic grades. EN 10088-3 gives 200 HB as the guidance maximum for annealed [430](https://www.laxconsteels.com/grades/aisi-430/) (1.4016) bar up to 100 mm, the same figure it gives the other standard ferritic grades. ASTM A240 limits annealed 430 plate and sheet to 183 HB or 89 HRB.

## Martensitic grades: annealed against hardened and tempered

Martensitic grades have the widest hardness range of any family. Annealed, they consist of spheroidised carbides in ferrite and are machinable. EN 10088-3 gives guidance maxima of 220 HB for [410](https://www.laxconsteels.com/grades/aisi-410/) (1.4006), 230 HB for [420](https://www.laxconsteels.com/grades/aisi-420/) (1.4021) and 295 HB for [431](https://www.laxconsteels.com/grades/aisi-431/) (1.4057). ASTM A276 sets binding maxima for its Condition A: 241 HB for hot finished 420 and 255 HB for cold finished 420, 285 HB for 431, and 269 HB for hot finished and 285 HB for cold finished 440C. Cold finishing raises the limit most in small diameters: for annealed bright bar of 1.4021, EN 10088-3 allows 290 HB up to 16 mm and 230 HB from 63 to 160 mm.

ASTM A276 also requires each martensitic grade to be capable of reaching a minimum hardness after a defined hardening treatment, the response to heat treatment: 35 HRC for 410 after air cooling from at least 955 degrees Celsius, 50 HRC for 420 after air cooling from at least 995 degrees Celsius, 40 HRC for 431 after oil quenching from at least 1,020 degrees Celsius, and 58 HRC for 440C after air cooling from at least 1,020 degrees Celsius. The requirement proves that the bar can harden. It is not the hardness in which the bar is delivered.

After quenching, the bar is tempered, and the tempering temperature sets the final hardness. Published producer data show 410 at about 388 HB after hardening and low-temperature tempering, falling to about 225 to 235 HB after tempering at 620 to 650 degrees Celsius. The same data show 420 at about 48 HRC after tempering near 230 degrees Celsius and about 23 HRC near 650 degrees Celsius. The same data for 410 record lower impact toughness and somewhat lower corrosion resistance after tempering between about 400 and 565 degrees Celsius, so that band is avoided. EN 10088-3 specifies its quenched and tempered conditions, such as +QT650 for 1.4006 and +QT800 for 1.4021, by tensile range rather than hardness. The free-machining grade 416 is ordered by hardness under ASTM A582: Condition A at 262 HB maximum, or Condition T, an intermediate temper, at 248 to 302 HB. At the top of the family, hardened and low-tempered 440C reaches about 58 to 60 HRC, the highest of the common martensitic grades, at the cost of toughness.

## Duplex grades

Duplex stainless steels are supplied solution annealed and quenched, and they have no hardening heat treatment. Their annealed hardness is still higher than that of austenitic grades, because nitrogen in solid solution and the fine-grained two-phase structure both strengthen the steel. EN 10088-3 gives guidance maxima of 270 HB for [2205](https://www.laxconsteels.com/grades/duplex-2205/) (1.4462) and 290 HB for [super duplex 2507](https://www.laxconsteels.com/grades/super-duplex-2507/) (1.4410) bar up to 160 mm, against 215 HB for 304. EN 10088-3 also sets the minimum 0.2 percent proof strength of 1.4462 at 450 MPa, more than twice the 190 MPa of 1.4301. ASTM A240 limits 2205 plate to 293 HB or 31 HRC and 2507 plate to 310 HB or 32 HRC.

Duplex hardness rises above the annealed level with cold work, or with the precipitation of intermetallic phases such as sigma during exposure between roughly 600 and 1,000 degrees Celsius. Sigma phase is hard and brittle and lowers toughness and corrosion resistance together; ASTM A923 detects it by metallographic, impact and corrosion tests, not by hardness. The structure and fabrication limits of the family are described in [duplex stainless steels](https://www.laxconsteels.com/what-are-duplex-stainless-steels-a-simplified-guide/).

## Precipitation hardening grades: Condition A and H900 to H1150

Precipitation hardening grades are the one family whose final hardness is set by an ageing treatment at low temperature, without a quench, after machining. ASTM A564 covers [17-4 PH](https://www.laxconsteels.com/grades/17-4-ph/) and [15-5 PH](https://www.laxconsteels.com/grades/15-5-ph/) bar. In Condition A, solution treated and not aged, the bar is held to 363 HB or 38 HRC at most. Each aged condition is named after its ageing temperature in degrees Fahrenheit and carries a minimum hardness. H900, aged at about 482 degrees Celsius, requires 388 HB or 40 HRC. The minimum then falls as the ageing temperature rises: 35 HRC for H1025, 31 HRC for H1100 and 28 HRC for H1150, aged at about 621 degrees Celsius. H1150M, a double treatment at 760 and then 621 degrees Celsius, requires 255 HB. The A564 conditions, with the minimum tensile and yield strength of each, are tabulated on the [precipitation hardening steels](https://www.laxconsteels.com/products/precipitation-hardening-steels/) page.

Lower hardness in this family buys toughness and resistance to stress corrosion cracking: H900 is the strongest and least resistant condition, H1150 and H1150M the toughest. Condition A is not a service condition, because unaged bar has reduced ductility and poor resistance to stress corrosion cracking, even when its hardness is acceptable. EN 10088-3 sets a guidance maximum of 360 HB for 1.4542, the EN equivalent of 17-4 PH, in the solution annealed condition, and specifies its aged conditions by tensile strength level. The mechanism of ageing is described in the [precipitation hardening article](https://www.laxconsteels.com/understanding-precipitation-hardening-stainless-steel-process-types-and-benefits/).

## Hardness limits in sour service

NACE MR0175 / ISO 15156 uses hardness as its main control against sulphide stress cracking in oil and gas equipment exposed to hydrogen sulphide, because hard, high-strength steel cracks most readily. ISO 15156-3 accepts austenitic grades such as 304 and 316 when solution annealed, free of cold work intended to raise strength, and at 22 HRC maximum. It accepts martensitic 410 and 420 at 22 HRC maximum, in the quenched and tempered conditions it defines (for 410, a second temper below the first), and limits their use by hydrogen sulphide partial pressure and pH. It accepts 17-4 PH and 15-5 PH only for listed components, in the double-aged H1150 condition (H1150D) or in H1150M, at 33 HRC maximum. The 2020 edition further restricts 17-4 PH used within the environmental limits of its table to applications where the sustained stress is no more than 50 percent of the specified minimum yield strength. For solution annealed wrought duplex, ISO 15156-3 sets a ferrite range rather than a hardness limit, while NACE MR0103, the refinery standard, limits duplex to 28 HRC. The structure of the standard and its environmental limits are set out in [NACE MR0175 / ISO 15156 and NORSOK M-650](https://www.laxconsteels.com/nace-mr0175-iso-15156-norsok-m-650/).

## Hardness and machinability

A martensitic stainless bar cuts much like a carbon steel of the same hardness, and above about 30 HRC it turns with much greater difficulty. Parts in 410, 420 and 431 are therefore machined annealed or highly tempered, then hardened, and finished by grinding where the hardness is high. An annealed 304 bar is soft, but it work hardens ahead of the cutting edge, so its machinability is limited by work hardening rather than by its starting hardness. The free-machining grades 303 and 416 add sulphur to break the chip, and ASTM A582 supplies both in Condition A at 262 HB maximum; they are described in [free-machining stainless steel](https://www.laxconsteels.com/free-machining-stainless-steel/). Precipitation hardening grades are machined in Condition A, at up to 38 HRC, and aged afterwards. With no quench, the part keeps its shape better than a quenched martensitic part. The heat treatments behind each condition are described in [heat treatment of steel](https://www.laxconsteels.com/heat-treatment-of-steel/).

## Hardness and condition of Laxcon Steels bar

Laxcon Steels supplies precipitation hardening bar in 17-4 PH, 15-5 PH, 1.4542 and 1.4594 to ASTM A564 and EN 10088-3, in Condition A or in the aged condition named in the order, from H900 to H1150, H1150D and H1150M, as listed on the [precipitation hardening steels](https://www.laxconsteels.com/products/precipitation-hardening-steels/) page. It rolls [hot rolled round bar](https://www.laxconsteels.com/products/hot-rolled-round-bars/) from 16 to 125 mm, heat treated by solution, soft or spheroidise annealing or by quenching and tempering, and lists it in grades including 304, 316, 430, 410, 420, 431, duplex 2205 and super duplex 2507; the families are set out in its [grade reference](https://www.laxconsteels.com/grades/). Mechanical testing is carried out in the company's own laboratory at Sanand, which holds NABL accreditation (certificate TC-12337) to ISO/IEC 17025:2017, as shown on the [quality](https://www.laxconsteels.com/quality/) page.

## Frequently asked questions

### What is the hardness of 304 stainless steel?

Annealed 304 bar is held to 215 HB maximum, for guidance, by EN 10088-3. Annealed 304 plate and sheet is limited to 201 HB or 92 HRB by ASTM A240. Cold working raises the hardness of 304 well above these values, because the grade cannot be hardened by heat treatment and work hardens rapidly.

### What is the hardness of 316 stainless steel?

Annealed 316 bar has the same 215 HB guidance maximum as 304 in EN 10088-3. ASTM A240 limits annealed 316 plate and sheet to 217 HB or 95 HRB, slightly above 304 because molybdenum strengthens the solid solution. Like 304, 316 is hardened only by cold work.

### How hard is 17-4 PH stainless steel?

Under ASTM A564, 17-4 PH bar in Condition A is limited to 363 HB or 38 HRC. After ageing it must reach at least 40 HRC in H900, falling to at least 28 HRC in H1150. The condition is therefore part of the material specification, because hardness, strength and resistance to stress corrosion cracking all change with it.

### What hardness can 420 stainless steel reach?

ASTM A276 requires 420 to reach at least 50 HRC when air cooled from 995 degrees Celsius or above in its response-to-heat-treatment test. Low-temperature tempering keeps it near that level; tempering near 650 degrees Celsius brings it down to about 23 HRC in published producer data. Annealed hot finished 420 bar is limited to 241 HB.

## Sources

- EN 10088-3, Stainless steels, Part 3: technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes.
- ASTM A276/A276M, Standard Specification for Stainless Steel Bars and Shapes.
- ASTM A564/A564M, Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes.
- ASTM A582/A582M, Standard Specification for Free-Machining Stainless Steel Bars.
- ASTM A240/A240M, Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications.
- ASTM A193/A193M, Standard Specification for Alloy-Steel and Stainless Steel Bolting for High Temperature or High Pressure Service and Other Special Purpose Applications.
- ASTM A923, Standard Test Methods for Detecting Detrimental Intermetallic Phase in Duplex Austenitic/Ferritic Stainless Steels.
- NACE MR0175 / ISO 15156-2 and ISO 15156-3, materials for use in H2S-containing environments in oil and gas production.
- NACE MR0103 / ISO 17945, metallic materials resistant to sulfide stress cracking in corrosive petroleum refining environments.
- ISO 18265 and ASTM E140, hardness conversion tables for metallic materials.

![Precipitation hardening stainless steel bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-precipitation-hardening-bars.webp)

Enquire about **Precipitation Hardening Steels**

First name Last name Email Phone Company Location

Product

- Bright Bars
- Precision Shaft Quality (PSQ) Bars
- Pipes and Tubes
- Hexagonal Bright Bars
- Square Bright Bars
- Cold-Drawn Flat Bars
- Forged & Proof Machined Bars
- HRAP Flat Bars
- HRAP Equal Angles
- HRAP Unequal Angles
- Threaded Bars
- Hot Rolled Round Cornered Squares (RCS) Bars
- Hot Rolled Round Bars
- Continuous Cast Billets / Blooms
- Channels
- Forging Quality Ingots
- Precipitation Hardening Steels
- Duplex Steel
- T-Profile
- Others

Message

\* Required

## From the Mill

- [![Precipitation hardening stainless steel bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-precipitation-hardening-bars.webp) Precipitation Hardening Steels](https://www.laxconsteels.com/products/precipitation-hardening-steels/)
- [![Stainless steel hot rolled round bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-hot-rolled-round-bars.webp) Hot Rolled Round Bars 16 mm to 125 mm](https://www.laxconsteels.com/products/hot-rolled-round-bars/)
- [![Optical emission spectrometer used to certify grade composition](https://www.laxconsteels.com/images/quality/laxcon-steels-optical-emission-spectrometer.webp) Grade reference](https://www.laxconsteels.com/grades/)