# AISI 904L

*[Home](https://www.laxconsteels.com/) > [Grades](https://www.laxconsteels.com/grades/) > [Austenitic grades](https://www.laxconsteels.com/grades/austenitic/) > AISI 904L*

A high-alloy austenitic stainless steel with copper, for sulphuric acid and chloride service.

AISI 904 L UNS N08904 EN 1.4539

## What is AISI 904L?

AISI 904L is a high-alloy, low-carbon austenitic stainless steel with additions of molybdenum and copper. It contains 19.0 to 23.0 percent chromium, 23.0 to 28.0 percent nickel, 4.0 to 5.0 percent molybdenum and 1.0 to 2.0 percent copper. Carbon is limited to 0.02 percent. The grade was developed for resistance to sulphuric acid. Copper is the element that provides this resistance. Molybdenum and chromium provide resistance to chloride pitting and crevice corrosion.

The nickel content of AISI 904L is roughly twice that of AISI 316. Nickel at this level keeps the structure fully austenitic, without ferrite, and raises resistance to chloride stress corrosion cracking above that of the standard austenitic grades. The grade is non-magnetic in all conditions. Atlas Steels places its corrosion performance in most environments between AISI 316L and the 6 percent molybdenum super austenitic grades.

AISI 904L is not hardenable by heat treatment. The specifications give its properties in the solution annealed condition. Strength can be raised only by cold work.

Laxcon Steels lists AISI 904L in its grades reference as an austenitic grade. The same steel is written 904L, SS 904L, 1.4539 and N08904.

## What is the chemical composition of AISI 904L?

Composition limits in weight percent are carbon 0.02 maximum, manganese 2.0 maximum, sulphur 0.03 maximum, phosphorus 0.045 maximum, silicon 1.0 maximum, chromium 19.0 to 23.0, nickel 23.0 to 28.0, molybdenum 4.0 to 5.0 and copper 1.0 to 2.0.

Composition, weight percent, balance iron.

| Element | Symbol | Minimum % | Maximum % |
| --- | --- | --- | --- |
| Carbon | C |  | 0.02 |
| Manganese | Mn |  | 2.0 |
| Sulphur | S |  | 0.03 |
| Phosphorus | P |  | 0.045 |
| Silicon | Si |  | 1.0 |
| Chromium | Cr | 19.0 | 23.0 |
| Nickel | Ni | 23.0 | 28.0 |
| Molybdenum | Mo | 4.0 | 5.0 |
| Copper | Cu | 1.0 | 2.0 |

## What is AISI 904L equivalent to in other standards?

UNS N08904 EN number 1.4539

Equivalence means nearest counterpart, not identity: each standards body sets its own composition window, so check the limits of the standard actually named on the order before substituting.

## What is the PREN of AISI 904L?

**32.2** PREN at the specified minima **39.5** PREN at the specified maxima

Computed by Laxcon Steels from the composition above as PREN = Cr + 3.3Mo + 16N, the relationship published in Practical Guidelines for the Fabrication of Duplex Stainless Steels (International Molybdenum Association, third edition, 2014). The first figure uses the minimum specified chromium, molybdenum and nitrogen, so it is the floor for a conforming heat rather than a typical value; the second uses the maxima, so the two together are the width of the band one compliant grade allows. PREN ranks resistance to chloride pitting and nothing else: it does not predict crevice corrosion, stress corrosion cracking or service life, and it is not a substitute for a corrosion test. The [pitting resistance reference](https://www.laxconsteels.com/grades/pitting-resistance/) carries the full table and the caveats.

## Mechanical properties of AISI 904L

ASTM A240 specifies minimum properties for annealed plate in UNS N08904. These are 490 MPa tensile strength, 220 MPa yield strength at 0.2 percent offset and 35 percent elongation in 50 mm, with a maximum hardness of 90 HRB. Bar and wire in the same alloy are specified in ASTM B649. Atlas Steels notes that the bar, pipe and tube specifications give similar but not necessarily identical properties to the plate specification. ATI reports typical annealed values of about 605 MPa tensile strength, 270 MPa yield strength, 50 percent elongation and 150 HB.

The yield strength of AISI 904L is close to that of AISI 316 and well below that of the duplex grades. Its minimum yield strength is about half the 450 MPa specified for duplex 2205 bar. A component in 904L therefore needs a thicker section than the same component in 2205 at the same design stress.

The ASME Boiler and Pressure Vessel Code, Section VIII, assigns allowable stresses to UNS N08904 up to 371 degrees Celsius. ATI lists the maximum allowable stress as 123 MPa at 38 degrees Celsius and 79 MPa at 371 degrees Celsius. The density is about 8,000 kg per cubic metre and the elastic modulus about 200 GPa, according to Atlas Steels.

## Corrosion behaviour of AISI 904L

AISI 904L resists sulphuric acid over a wider range of concentration and temperature than AISI 316. Atlas Steels identifies the mid-concentration range of sulphuric acid as the range in which the copper addition has the largest effect. ATI reports a corrosion rate of 2.57 mm per year for 904L in boiling 10 percent sulphuric acid, against 16.2 mm per year for 316. In boiling 1 percent hydrochloric acid, the corresponding rates are 0.55 and 5.74 mm per year. The grade also resists phosphoric and acetic acids and many reducing media.

Resistance to chloride crevice corrosion is ranked by the ferric chloride test of ASTM G48. In ATI's ranking, the onset temperature for crevice attack is about 18 degrees Celsius for 904L, minus 3 degrees Celsius for 316, 2 degrees Celsius for 317 and 45 degrees Celsius for the 6 percent molybdenum grade AL-6XN. These figures rank the alloys under one test procedure. They are not service temperature limits.

Chloride stress corrosion cracking resistance rises with nickel content. In ATI's U-bend tests to 1,000 hours, 904L did not crack in boiling 26 percent sodium chloride, a solution in which 316 cracked. Both grades cracked in boiling 42 percent magnesium chloride. The grade therefore has improved resistance to chloride stress corrosion cracking but is not immune.

## Seawater and high-chloride service

Atlas Steels gives AISI 904L a pitting resistance equivalent of about 35 and states that this level indicates good resistance to warm seawater and other high-chloride environments. ATI states that the grade is not totally resistant to aerated seawater and recommends it where some degree of attack can be tolerated, for example in seawater heat exchanger tubesheets. The two statements describe the same position: 904L is above 316L in seawater and below the alloys intended for full immersion.

In pitting resistance, AISI 904L and duplex 2205 overlap. Atlas Steels rates their corrosion resistance as very similar and notes that 2205 has the higher strength and the lower cost. Super duplex 2507 and the 6 percent molybdenum super austenitic grades are rated above 904L for seawater and for crevices under deposits.

## Heat treatment, welding and fabrication

Solution treatment is carried out at 1,090 to 1,175 degrees Celsius followed by rapid cooling, according to Atlas Steels; ATI gives 1,095 to 1,150 degrees Celsius. Like other highly alloyed austenitic grades, 904L is structurally unstable at elevated temperature. Sigma and other brittle phases precipitate during prolonged exposure, so the grade is not used above about 550 degrees Celsius.

AISI 904L can be welded by all standard fusion processes. The weld metal solidifies fully austenitic, which makes it susceptible to hot cracking in restrained joints. No preheat is applied, and post-weld heat treatment is normally not required. ATI recommends an overmatched filler, more highly alloyed than the parent metal, for welds exposed to corrosive service. Matching 904L filler is used where the environment is mildly corrosive.

AISI 904L is a high-purity, low-sulphur grade. It machines less readily than grades with sulphur added for machinability, although standard techniques apply. It cold forms like the standard austenitic grades but requires higher forming loads. Solution annealing after cold work is considered where severe stress corrosion cracking conditions are expected.

## Applications and designations

Typical applications include process plant for sulphuric, phosphoric and acetic acids, pulp and paper processing, gas scrubbing plant and utility flue gas scrubbers, seawater cooling equipment, oil refinery components, fertiliser production and wires for electrostatic precipitators.

Under EN 10088, AISI 904L corresponds to material number 1.4539 with the name X1NiCrMoCu25-20-5. Its UNS number is N08904, and the Swedish designation is SS 2562. Purchasers also write the grade as 904L, SS 904L or SS904L. Because the UNS number begins with N, some specifications classify the alloy with the nickel alloys rather than with the stainless steels; ASTM covers its bar under B649 rather than under the stainless bar specifications. The standard and designation stated on the order determine the applicable requirements.

## Where AISI 904L is not the right choice

AISI 904L is not an economical choice where duplex 2205 meets the corrosion requirement. Its nickel and molybdenum contents make it costly, and Atlas Steels notes that many applications once filled by 904L are now filled at lower cost by 2205, which also has about twice the yield strength. The exceptions are service above about 300 degrees Celsius, where duplex grades embrittle, and parts that require severe forming.

AISI 904L is also unsuitable for full immersion in warm aerated seawater and for crevices under marine deposits, where super duplex 2507 or a 6 percent molybdenum super austenitic grade is specified. It has lower resistance than molybdenum-free grades such as 304L and 310L in aggressive nitric acid. Prolonged service above about 550 degrees Celsius is excluded because of brittle phase precipitation. Applications that depend on high strength or hardness require a duplex, martensitic or precipitation hardening grade, since 904L cannot be hardened by heat treatment.

## Other austenitic grades

[**AISI 304** The general purpose austenitic stainless steel](https://www.laxconsteels.com/grades/aisi-304/) [**AISI 304L** The low-carbon version of AISI 304](https://www.laxconsteels.com/grades/aisi-304l/) [**AISI 304H** The high-carbon version of AISI 304](https://www.laxconsteels.com/grades/aisi-304h/) [**AISI 316** The molybdenum-bearing austenitic grade](https://www.laxconsteels.com/grades/aisi-316/) [**AISI 316L** The low-carbon version of AISI 316](https://www.laxconsteels.com/grades/aisi-316l/) [**AISI 316Ti** AISI 316 stabilised with titanium](https://www.laxconsteels.com/grades/aisi-316ti/)

Composition from the Laxcon Steels grade reference, which covers 500+ grades: see [AISI 904 L in the full table](https://www.laxconsteels.com/grades/#aisi-904-l), the [austenitic family](https://www.laxconsteels.com/grades/austenitic/), or the [equivalents reference](https://www.laxconsteels.com/grades/equivalents/).