title: "ASTM A262: Intergranular Corrosion Tests for Stainless"
source: "https://www.laxconsteels.com/astm-a262-intergranular-corrosion-tests/"
description: "ASTM A262 Practices A, B, C, E and F and ISO 3651-2 explained: the oxalic acid etch, Streicher, Huey and Strauss tests, sensitising treatment and limits."
---
# Intergranular Corrosion Testing of Stainless Steel: ASTM A262 Practices A to F and ISO 3651-2

Send an enquiry

9 min read

An intergranular corrosion test is a laboratory test that shows whether a stainless steel is susceptible to attack along its grain boundaries. A prepared specimen is exposed to a hot acid, or etched in an electrolyte, chosen to dissolve chromium-depleted metal at the boundaries far faster than the grains themselves. The result is a corrosion rate, a crack pattern after bending, or a classification of the etched microstructure. ASTM A262 is the standard set of such tests for austenitic stainless steels, and its current edition, A262-26, replaced A262-15 in 2026. It contains five practices, lettered A, B, C, E and F. ISO 3651-1 and ISO 3651-2 are the international counterparts, adopted in Europe as EN ISO 3651-1 and EN ISO 3651-2. The ferritic and duplex stainless steels have their own standards, ASTM A763 and ASTM A923. The common shorthand for all of these is the IGC test.

## What the tests detect

An austenitic stainless steel that spends time in the range of roughly 425 to 860 degrees Celsius can precipitate chromium carbide at its grain boundaries. Each carbide takes its chromium from a thin band of metal beside the boundary, and that band can lose the passive film the bulk of the steel keeps. The condition is called sensitisation, and the attack it permits is intergranular corrosion; beside a weld it is known as weld decay. The [corrosion of stainless steel](https://www.laxconsteels.com/corrosion-of-stainless-steel/) article sets out the mechanism, and the [304L and 316L](https://www.laxconsteels.com/304-vs-304l-and-316-vs-316l/) article explains how low carbon prevents it. The tests answer a narrow question: whether the sample carries chromium-depleted boundaries, or in some tests other boundary phases, that an aggressive solution can find. ASTM A262 states that its results do not necessarily predict performance in other corrosive environments, and give no basis for predicting resistance to other forms of corrosion, such as general corrosion, pitting or stress corrosion cracking.

## Scope of ASTM A262

ASTM A262, Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels, covers one etch test and four hot acid immersion tests. The etch test, Practice A, is a rapid screen. Three of the immersion tests, Practices B, C and F, are evaluated by loss of mass and give a quantitative corrosion rate. The fourth, Practice E, is evaluated by bending the exposed specimen and looking for fissures, and it classifies a specimen only as acceptable or not acceptable.

The practices differ in how strongly they oxidise, and so in what they reveal. A mildly oxidising solution dissolves only metal that has lost chromium; a strongly oxidising one also attacks boundaries that carry intermetallic phases. Earlier editions of A262 noted in their scope that in most cases Practice E or Practice B, combined with the etch of Practice A, gives the information needed in the shortest time. The current edition places its guidance on choosing a practice in an appendix.

## Practice A: the oxalic acid etch test

Practice A classifies the etched microstructure of a polished cross-section. The specimen is made the anode in a 10 percent solution of oxalic acid and etched electrolytically, in common laboratory practice for about one and a half minutes at a current density of about 1 ampere per square centimetre. Chromium carbide at the boundaries etches far faster than the matrix, so a sensitised boundary appears under the microscope as a dark trench. The structures are named by their appearance. A step structure shows only steps between grains of different orientation and no trenches. A dual structure shows some trenches among the steps. A ditch structure shows continuous trenches along the boundaries. The standard also names four further classes: isolated ferrite, interdendritic ditches, and two forms of end-grain pitting.

The test is a screen, not a verdict. A262 classifies each specimen as acceptable or suspect. An acceptable structure releases the lot without the longer immersion test, and a suspect structure sends the specimen on to the hot acid practice the specification names. The etch can accept material; it cannot reject it. It applies only to the grades listed in the individual hot acid practices, and it responds to chromium carbide rather than to other boundary phases.

## Practices B and C: the Streicher and Huey tests

Practice B, the ferric sulphate and sulphuric acid test, is known as the Streicher test. The specimen is boiled for 120 hours in a solution of about 50 percent sulphuric acid with ferric sulphate added as the oxidiser. Ferric sulphate holds the steel at a potential where chromium-depleted metal dissolves and the passive grains do not. The mass lost over the exposure is converted to a corrosion rate. Practice B detects susceptibility caused by chromium carbide, and in the stabilised and the cast molybdenum-bearing grades it also responds to sigma phase. It is widely applied to the 300 series grades, including the molybdenum-bearing ones.

Practice C, the nitric acid test, is the Huey test. The specimen is boiled in 65 percent nitric acid for five periods of 48 hours, 240 hours in all, and weighed after each period. Boiling nitric acid is strongly oxidising. It attacks chromium-depleted zones, and it also attacks boundaries carrying sigma phase and other intermetallic precipitates, which a milder test passes. In some wrought grades, attack associated with sigma phase raises the corrosion rate in nitric acid alone, so the Huey test can reveal susceptibility that Practice E, and in those grades Practice B, does not. Earlier editions of A262 required Practice C for stabilised and molybdenum-bearing grades intended for nitric acid service, and for any grade that may suffer end-grain attack in that service. Each weight-loss practice reports a corrosion rate; the maximum rate it is judged against comes from the product specification or the purchase order.

## Practice E: the Strauss test and the bend

Practice E, the copper, copper sulphate and 16 percent sulphuric acid test, is known as the Strauss test. The specimen is boiled in a solution of 16 percent sulphuric acid and copper sulphate, in contact with metallic copper, for 15 hours. Earlier editions of A262 set 24 hours. The copper in contact with the specimen fixes its potential in a narrow band where chromium-depleted metal is active and the rest of the steel stays passive, so the test is selective for carbide-related sensitisation and largely blind to intermetallic phases.

Practice E is not judged by loss of mass. Instead the specimen is bent through 180 degrees, normally over a mandrel whose diameter equals the specimen thickness, with the exposed surface on the outside of the bend. The bent surface is examined at low magnification. Intergranular fissures mean the material is susceptible. Cracks that start only at the edges of the specimen, and the roughened surface known as orange peel, are not counted as intergranular attack.

## Practice F, and the missing Practice D

Practice F, the copper, copper sulphate and 50 percent sulphuric acid test, is a more severe relative of Practice E. The specimen is boiled for 120 hours and evaluated by loss of mass. A262 applies it to molybdenum-bearing austenitic steels, and in practice it is used mainly on cast alloys of the 316 type. There is no Practice D in the current edition. A practice once published under that letter was deleted, and the remaining letters were kept as they were rather than renumbered, which is why A262 runs A, B, C, E and F.

## The ASTM A262 practices compared

Practice A is the oxalic acid etch test, Practice B the Streicher test, Practice C the Huey test, Practice E the Strauss test, and Practice F the copper sulphate and 50 percent sulphuric acid test. The first table gives the medium and the exposure of each practice.

*ASTM A262 intergranular corrosion practices for austenitic stainless steel: medium and exposure*

| Practice | Medium | Exposure |
| --- | --- | --- |
| A | 10 percent oxalic acid, electrolytic | Minutes |
| B | Boiling sulphuric acid with ferric sulphate | 120 hours |
| C | Boiling 65 percent nitric acid | Five periods of 48 hours |
| E | Boiling 16 percent sulphuric acid with copper sulphate and metallic copper | 15 hours |
| F | Boiling 50 percent sulphuric acid with copper sulphate and metallic copper | 120 hours |

Practice A is evaluated on the etch structure under the microscope, as acceptable or suspect. Practices B, C and F are evaluated by loss of mass, as a corrosion rate, and Practice E by a 180 degree bend, as fissures or none. The second table gives what each practice detects.

*ASTM A262 intergranular corrosion practices for austenitic stainless steel: what each detects*

| Practice | Detects |
| --- | --- |
| A | Chromium carbide at boundaries (screen only) |
| B | Chromium depletion from carbide; sigma in stabilised and cast molybdenum-bearing grades |
| C | Chromium depletion, sigma and other intermetallic phases |
| E | Chromium depletion from carbide |
| F | Chromium depletion in molybdenum-bearing, mainly cast, alloys |

## Sensitising heat treatment, and the L and stabilised grades

A specimen is tested in one of two states, and the state decides what the result means. A test on a standard carbon grade, such as [304](https://www.laxconsteels.com/grades/aisi-304/) or [316](https://www.laxconsteels.com/grades/aisi-316/) with up to 0.08 percent carbon, in the condition in which it was delivered shows whether the solution anneal and quench left the boundaries free of carbide. It does not show that the steel will stay so through welding.

The low-carbon grades, [304L](https://www.laxconsteels.com/grades/aisi-304l/) and [316L](https://www.laxconsteels.com/grades/aisi-316l/) with carbon held to 0.03 percent, and the stabilised grades, [321](https://www.laxconsteels.com/grades/aisi-321/) with titanium and [347](https://www.laxconsteels.com/grades/aisi-347/) with niobium, exist to resist sensitisation. Testing them as delivered would prove little, so A262 tests them after a deliberate sensitising treatment between 650 and 675 degrees Celsius, most often one hour at 675 degrees Celsius. The treatment stands in for the heat of a welding cycle, and a pass after it shows that the steel resists the carbide precipitation a weld would cause. A failure after it points to too much free carbon for the grade, or too little titanium or niobium to tie that carbon up.

The bar specifications use the same logic. ASTM A479, the specification for stainless steel bars and shapes for boilers and pressure vessels, carries an intergranular corrosion test as its supplementary requirement S2, which the purchaser specifies where intergranular attack is a concern and which is carried out on sensitised specimens. The [ASTM A276 and A479](https://www.laxconsteels.com/astm-a276-a479-stainless-steel-bar-specifications/) article describes the two bar specifications.

## ISO 3651-1 and ISO 3651-2

ISO 3651 is published in two parts, both in editions of 1998 that ISO confirmed in 2021 and marked for revision in 2025. ISO 3651-1 is the Huey test: austenitic and duplex stainless steels boiled in nitric acid and evaluated by loss of mass, the counterpart of A262 Practice C. In general it is not applied to molybdenum-bearing grades unless they are intended for nitric acid service.

ISO 3651-2 tests ferritic, austenitic and duplex stainless steels, cast, rolled, forged or as tube, in media containing sulphuric acid, for steels meant for mildly oxidising acids such as sulphuric and phosphoric acid. It has three methods.

- Method A: the 16 percent sulphuric acid and copper sulphate test, in contact with copper, the Monypenny Strauss test and the close counterpart of A262 Practice E.
- Method B: the 35 percent sulphuric acid and copper sulphate test, also with copper.
- Method C: the 40 percent sulphuric acid and ferric sulphate test, related to the Streicher test of A262 Practice B.

In all three methods the specimen is boiled in the solution and then bent, and the convex surface is examined for cracks caused by intergranular corrosion; a small-diameter tube is flattened instead. Method A boils the specimen for 20 hours, within a tolerance of 5 hours either way. Unless the product standard names the method, the parties agree on one, and an annex to the standard gives examples of the steels each method suits. The low-carbon steels, with carbon below 0.03 percent, and the stabilised steels are sensitised before testing. For austenitic and duplex steels the heat treatment is either 30 minutes at 700 degrees Celsius or 10 minutes at 650 degrees Celsius, each followed by water cooling, and the 700 degree treatment applies when the order names neither. A welded test piece, tested as welded, may replace the heat treatment by agreement. ISO 3651-2 Method A and A262 Practice E are close in chemistry but differ in sensitising treatment and exposure time, so a result under one is not a result under the other.

## Ferritic and duplex grades: ASTM A763 and ASTM A923

A262 is written for austenitic steels. Ferritic stainless steels sensitise under different thermal conditions, and ASTM A763 holds four practices for them, lettered W to Z: an oxalic acid etch used as a screen, a ferric sulphate and sulphuric acid test, and copper sulphate tests in 50 percent and in 16 percent sulphuric acid. Grades such as [430](https://www.laxconsteels.com/grades/aisi-430/) fall within it.

Duplex stainless steels such as [duplex 2205](https://www.laxconsteels.com/grades/duplex-2205/) and [super duplex 2507](https://www.laxconsteels.com/grades/super-duplex-2507/) raise a different question. Their low carbon and high chromium make carbide sensitisation a lesser concern, but slow cooling or a long hold in the range of roughly 600 to 1,000 degrees Celsius precipitates sigma and other intermetallic phases that cost both toughness and corrosion resistance. ASTM A923 detects those phases by three test methods: a sodium hydroxide etch classified under the microscope, a Charpy impact test, and a ferric chloride corrosion test. A923 does not identify which phase is present, and compliance with the composition and tensile requirements of a product specification does not show its absence. The [Charpy and Izod impact tests](https://www.laxconsteels.com/charpy-and-izod-impact-tests/) article describes the impact method, and ASTM A1084 holds similar methods for the lean duplex grades.

## Austenitic bar from Laxcon Steels

Laxcon Steels melts stainless steel at Sanand, Gujarat, where its melting shop refines by argon oxygen decarburisation (AOD) and vacuum oxygen decarburisation (VOD), the processes that take a melt down to the 0.03 percent carbon ceiling of the L grades. Its heat treatment shop holds three gas-fired, PLC-controlled solution annealing furnaces of 6 tonnes each and a 60 kilolitre water quenching tank, as set out on the [technology](https://www.laxconsteels.com/technology/) page. [Hot rolled round bar](https://www.laxconsteels.com/products/hot-rolled-round-bars/), from 16 to 125 mm, is rolled to order in grades including 304L, 316L, 316Ti, 321 and 347, with solution annealing among its heat treatment conditions and ASTM A479 among its governing standards. The bar pages for [304L](https://www.laxconsteels.com/products/hot-rolled-round-bars/aisi-304l/), [316L](https://www.laxconsteels.com/products/hot-rolled-round-bars/aisi-316l/) and [321](https://www.laxconsteels.com/products/hot-rolled-round-bars/aisi-321/) list the sizes and the weight per metre for each of those grades.

## Frequently asked questions

### What is ASTM A262 Practice E?

Practice E is the copper, copper sulphate and 16 percent sulphuric acid test, also called the Strauss test. A specimen is boiled in the solution, in contact with metallic copper, for 15 hours, then bent through 180 degrees and examined for intergranular fissures. Fissures mean the steel is susceptible to intergranular attack from chromium carbide.

### What is the difference between ASTM A262 Practice C and Practice E?

Practice C boils the specimen in 65 percent nitric acid for five 48-hour periods and measures the loss of mass. It detects chromium depletion and also intermetallic phases such as sigma. Practice E boils the specimen for 15 hours in a copper sulphate and sulphuric acid solution and judges it by a bend. It responds mainly to carbide-related sensitisation. Earlier editions of A262 required Practice C for stabilised and molybdenum-bearing steels intended for nitric acid service.

### Can the oxalic acid etch test reject material?

No. Practice A of ASTM A262 classifies a specimen as acceptable or suspect. An acceptable etch structure releases the material without a hot acid test; a suspect one requires the hot acid practice the specification names, and only that practice can show the material susceptible.

### Why are 304L and 316L sensitised before an intergranular corrosion test?

The low-carbon grades are made to resist sensitisation during welding, so a test in the delivered condition would prove little. ASTM A262 heats them between 650 and 675 degrees Celsius, most often for one hour at 675 degrees Celsius, before the acid exposure. A pass after that treatment shows that the steel resists the kind of sensitisation a welding cycle causes.

## Sources

- ASTM A262-26 and A262-15 (reapproved 2021), Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels: the five practices, their evaluation, the scope cautions and the etch structure classes.
- ASTM A763, Standard Practices for Detecting Susceptibility to Intergranular Attack in Ferritic Stainless Steels: Practices W, X, Y and Z.
- ASTM A923, Standard Test Methods for Detecting Detrimental Intermetallic Phase in Duplex Austenitic/Ferritic Stainless Steels: Test Methods A, B and C.
- ASTM A1084, Standard Test Method for Detecting Detrimental Phases in Lean Duplex Austenitic/Ferritic Stainless Steels.
- ASTM A479/A479M, Standard Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels: supplementary requirement S2.
- ISO 3651-1:1998, Determination of resistance to intergranular corrosion of stainless steels, Part 1: Austenitic and ferritic-austenitic (duplex) stainless steels, Corrosion test in nitric acid medium by measurement of loss in mass (Huey test).
- ISO 3651-2:1998, Determination of resistance to intergranular corrosion of stainless steels, Part 2: Ferritic, austenitic and ferritic-austenitic (duplex) stainless steels, Corrosion test in media containing sulfuric acid.

![Stainless steel hot rolled round bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-hot-rolled-round-bars.webp)

Enquire about **Hot Rolled Round Bars**

First name Last name Email Phone Company Location

Product

- Bright Bars
- Precision Shaft Quality (PSQ) Bars
- Pipes and Tubes
- Hexagonal Bright Bars
- Square Bright Bars
- Cold-Drawn Flat Bars
- Forged & Proof Machined Bars
- HRAP Flat Bars
- HRAP Equal Angles
- HRAP Unequal Angles
- Threaded Bars
- Hot Rolled Round Cornered Squares (RCS) Bars
- Hot Rolled Round Bars
- Continuous Cast Billets / Blooms
- Channels
- Forging Quality Ingots
- Precipitation Hardening Steels
- Duplex Steel
- T-Profile
- Others

Message

\* Required

## From the Mill

- [![Stainless steel hot rolled round bars produced by Laxcon Steels](https://www.laxconsteels.com/images/products/stainless-steel-hot-rolled-round-bars.webp) Hot Rolled Round Bars 16 mm to 125 mm](https://www.laxconsteels.com/products/hot-rolled-round-bars/)
- [![Optical emission spectrometer used to certify grade composition](https://www.laxconsteels.com/images/quality/laxcon-steels-optical-emission-spectrometer.webp) Grade reference](https://www.laxconsteels.com/grades/)